CHEMICAL PROBLEMS 2018 no. 4 (16) ISSN 2221-8688
505
UOT 544.23
OPTIMAL CONDITIONS FOR GRAFT RADICAL COPOLYMERIZATION OF N-VINYLPIRROLIDON AND 4-VINYLPIRIDINE INTO CHITOSAN
Sh.Z. Tapdigov*, N.A. Zeynalov*, D.B. Tagiyev*, S.F. Safaraliyeva*, E.M. Gasimov#, M.Kh. Hasanova*, A.F. Nuraliyev±, C.A. Sultanov*
'Institute Catalysis and Inorganic Chemistry Azerbaijan National Academy of Sciences H.Javid ave., 113, Baku AZ1143, Azerbaijan Republic; e-mail: [email protected] # Azerbaijan Medical University, Department of Surgery and Anaesthesiology S.Vurgun, 167, Baku AZ 1022, Azerbaijan Republic; e-mail: [email protected] ± Institute of Physics National Academy of Sciences ofAzerbaijan H.Javid ave., 33, Baku AZ 1143, Azerbaijan Republic; e-mail: azhep@ physics.ab.az
Received 21.09.2018
In our study, new natural-synthetic, cross-linked copolymers were obtained by radical copolymerization of chitosan in the presence of 4-vinylpyridine and N-vinylpyrrolidone. In order to cross-link 4-vinylpyridine and N-vinylpyrrolidone to chitosan, the radical co-polymerization with azobisanobutyronitrile initiator were performed in the homogeneous phase in the presence of monomers. The combined effects of the major parameters to the cross-linked radical copolymerization were studied systematically. The cross-linking degree of the monomers to chitosan (G) and dependence of cross-linking effectiveness (E) upon temperature, amount of chitosan, concentration of inisiator, solvent ratio, reaction time and concentration of monomers were studied. It revealed that G = 258% and E = 17-19% were max. at 60-700C, within 150 min., in the cross-linked copolymerization of 0.35 g chitosan with 2.4 mol/l of N-vinylpyrrolidone and 0.2 mol/l of 4-vinylpyridine in the presence of 75 ml 2% CH3COOH as a solvent, and the estimated degree of homopolymerization at minimum 18-20%. Through the use of 1H NMR, FTIR, SEM, X-Ray and thermogravimetric analysis methods, the mechanism of radical cross-linked copolymerization was proposed on the basis of the cyclic breakdown of chitosan. Keywords: chitosan; graft copolymer; N-vinylpyrrolidone; 4-vinylpyridine; radical polymerization. DOI: https://doi.org/10.32737/2221-8688-2018-4-505-513
INTRODUCTION
The modification of cross-linked copolymerization of natural polymers is a perfect way of obtaining materials with new properties. This method involves the acquisition of a new generation of biopolymers by adding different functional groups to macromolecules. Thus, such natural -synthetic cross-lnked materials are considered to be irreplaceable smart nanogels in medicine for drug delivery, genetic engineering, membrane conductivity, and tissues [1-4]. Chitosan from from deacetylation of Chitin is polyaminosaccharide which is residues of P-(1,4) -2-amino-2-deoxy- D-glucosamine and P- (1,4) -N-acetyl D-glucosamine [5-8]. The free amine groups in chitosan provide its solubility in acidic solutions which forms
positive charges on the polysaccharide macromolecule. Such positive charges allow chitosan and its modifications attract negative-charged drugs, proteins, bacteria and fungi [911]. It is possible to obtain different chitosan cross-linked polymers by radical polymerization of vinyl monomers in the homogeneous and heterogeneous phase in the presence of the chitosan as initiator. The radical polymerization reactions were analysed on various vinyl monomers such as, acrylnitrile, vinylacetate, methyl acrylate, methyl methacrylate, acrylic acid, acrylamide, vinylpyridines, vinylpyrrolidone, isopropyl acrylamide, etc. in the presence of different initiators [12-14]. Stimulating sysmens such as (NH4)Ce(NO3)6, K2S2O8, (NH4O2S2O8, tributyl
borane, Fenton's reagent (Fe2++H2O2), 2,2-azobis (2-methylpropionnitrile), UV radiation, microwave radiation, etc. were used as initiator [15-16]. Also, the homogeneous cross-linking process of vinylpyrrolidone to chitosan along with the presence of potassium persulfate as redox initiator have been examined to reach 290% cross-linking. It found that the water solubility of the product from the cross-linking of vinylpyrrolidone to chitosan decreases. The same is observed in organic and inorganic solvents, as well as in diluted acitic solutions. The HCl solubility increased after formation of a complex of chitosan with copper ion. This is related to the
formation of coordination bond with the amine group. In the present paper, the radical cross-linking copolymerization was performed concurrently with 4-vinylpyridine, N-vinylpyrrolidone and 2-azobisisobutyronitrile (AIBN) initiator to 150-300 kDa molecular weight chitosan. The effect of temperature, the amount of chitosan, the concentration of initiator, the volume of the solvent, the reaction time and the effectiveness of the monomers' concentration were studied and the optimum value of the cross-linking were determined. The mechanism of cross-linking reaction was examined through the use of FTIR and 1H, NMR spectroscopy methods.
EXPERIMENTAL
Samples
Chitosan Mn=35 kDa (deacetylating degree 85-87%), acetate acid (Glacial), ethanol (95%), acetone (residue analysis, >99.9%), diethyl ether (contains 1 ppm BHT as inhibitor, anhydrous, >99.7%) from Sigma-Aldrich. 4-vinylpyridine assay 95-96%,(bp 62-65 °C/15 mmHg, ri 20/D 1.549) and N-vinypyrrolidone assay >99% (bp 94 °C/11 mmHg, n20/D 1.512) from Acros Organics had been distilled just before the use. Initiators of AIBN came to be analytical grade reagents from Fluka chemicals. All solvents came from Aldrich and were purified by distillation, according to the conventional methods.
Grafting reactions, Swelling measurements and Quaternization.
1.5 g chitosan which is dried at 40-50 0C for 24 hours suspended in 150 ml of 2% CH3COOH. After 1-2 hours complete mixing, 2 mL of newly distilled monomers are added to the solution in 1:1 mol ratio and continuously stirred for 30 minutes. The reaction medium is coupled to a 650C water thermostat and the reaction performed in terms
of inert gas-N2 environment in the 0.15 mol/l AIBN concentration for 2 hours. Following an appropriate period, the solution is brought to pH = 10-11 by adding 1M KOH after which the product precipitates. Cross-linked copolymer is filtered, washed 2-3 times with water, alcohol and acetone (to clean from poly-4-vinylpyridine, poly-N-vinylpyrrolidone and monomers it is washed with diethyl ether for 2 days in Soxhlet). Cross-linked copolymer sample is dried to a constant weight at 40-500C. The yield is 78-86%. Swelling measurements were carried out in the distilled water, pH 6.5, acidic buffer pH 3.4, and in the basic buffer at pH=10 and at a room temperature. A well-known weight of the dry sample was placed into a tea-bag and immersed in the aqueous medium. In a while, the bag was taken out and hung for 5-10 min to eliminate excess unabsorbed water, and then weighed. The degree of swelling was calculated using the relation (W-W0)/W0*100 where W and W0 are the weight of the swollen and dry samples, respectively. Quaternization of chitosan and its grafted copolymers was achieved by heating the samples with dimethyl sulfate in the presence of NaOH.
RESULTS AND DISCUSSION
By varying the nature of the monomers and various parameters of cross-linking it is possible to change the hydrophobicity of the chitosan, which makes it possible to diversify with antibacterial properties. Systematically, in terms of the cross-linking rate G% 4-vinylpyridine and N-vinylpyrrolidone to chitosan, the percentage of
its use depending on a specific purpose. Another interesting change was the quaternization of cross-linked chitosan copolymer, which can be used as a material hopolymer (% H) and the cross-linking efficiency E% are investigated and determined according to the following expression:
w., - W, W. -Wa w, - w.
G% = —-- X 100, H % = —-- X 100, E% = —-- X 100
Wx W3 Wa
where W1, W2, W3 and W4 are the total amount of initial chitosan, the mass of cross-linked copolymer product after extraction, the total amount of N-vinylpyrrolidone and 4-vinylpyridine monomers, as well as the pre-extraction mass of cross-linked copolymer with grams, respectively.
The changes in the hydrophobicity of cross-linked copolymerization reaction are made depending on the molar ratio of monomer determined by using hydrophilic and hydrophobic monomers. Initially, cross-linked copolymerization reaction was determined depending on the amount of chitosan. Results are shown in Fig. 1.
Fig. 1. The effect of chitosan on cross-linking. VP = 2 ml, 4VP = 2 ml, Solvent = 10 ml, AIBN = 0.01 mol/l, T = 700C, t = 120 min.
As is seen from Fig. 1, the degree of radical cross-linked copolymerization of chitosan was max. in the amount of 0.3-0.35 g. High amounts of chitosan reduce the degree of cross-linking which is undesirable. We assign the objective to obtain a new characteristic copolymer together with monomer residues added to chitosan. Then, the copolymerization was carried out depending on the volume of
another parameter solvent. Results are shown in Fig.2.
It was determined that the cross-linking is sufficient by 85-90% in 75 ml of the solvent. Note that the rinse of the reaction medium reduces the interaction of active centers which indicates a decrease in the cross-linking effectivity.
Fig. 2. Effect of the solution volume to the cross-linking. mchitosan =0.35 g, VP=2 ml, 4VP=2 ml, t=120 min, T=700C, AIBN=0.01 mol/l.
Next, the impact of the initiator concentration process was examined, and the results which gives rise to active centers in the obtained are cited in Fig.3.
250
01 01 200
on {LI "U LU 150 /
100 /
■O c 50
x 0 . —_
ID 0 0.2 0.4 0.6
Concentration of initiator, mol/l
Fig. 3. Influence of incinerator concentration on cross-linking where mchitosan= 0.35 g, VP=2 ml, 4VP=2 ml, t=120 min, T=700C, Solvent=75 ml.
As is apparent from the diagram above, the radical cross-linking copolymerization reaction in 0.1-0.2 mol/l concentrated solution of initiator is effective and characterized by more than 200% cross-linking degree. This proves that the process is more active with the radical mechanism together with the majority of active centers which is due to the process acceleration. However, increased
concentration of the initiator which leads the reaction towards the homopolymerization of more monomers is undesirable. From this point of view, using 0.15 mol/l of the initiator can be optimally acceptable for copolymerization. The effect of the below parameter is the concentration of monomers (Fig.4) which led to more interesting results. It
revealed that the hydrophobicity of cross-linked copolymer increases with the amount of N-vinylpyrrolidone residues as compared to chitosan for a certain amount. This can be explained by the increase of hydrogen, hydrophobic, electrostatic and intermolecular type interactions due to the increase of polyar groups in the cross-linked copolymer. The increased amount of hydrophobic monomer, 4-vinylpyridine leads to a certain degree of hydrophilicity and then declines sharply.
This is primarily caused by the easy ionization, as well as the polarization of functional groups due to the decrease between macromolecular interactions [17].
Fig. 4. Influence of monomers molar ratio to cross-linking mchitosan 0.35 g, t=120 minutes, T=700C, AIBN=0.15 mol/l, Solvent=75 ml.
The predominance of the subsequent 4-vinylpyridine barks leads to greater hydrophobicity of cross-linked copolymer. This feature may limit its application as the most advantageous system based on the
mixture of 0.2 mol/l N-vinylpyrrolidone and 2.4 mol/l 4-vinylpyridine. Subsequently, the time dependence of the process (Fig. 5) was studied by keeping monomers molar ratio constant.
300
0 100 200 300 400
Duration of reaction, min.
Fig.5. Influence of reaction time on cross-linking. mchitosan 0.35 g, VP = 2.4 mol/l, 4VP=0.2 mol/l, T=700C, AIBN=0.15 mol/l, Solvent=75 ml.
As is seen from Fig.5, the duration of the cross-linked copolymerization reaction is 150 minute. The additional reaction time leads to outer processes, including the recombination of obtained macroradical s and the fall in the cross-linking degree and effectiveness. Despite the stabilization of these parameters after 200 min., it may take 100-150 min. with max. cross-linking degree without applying additional energy. Finally, the temperature dependence of the radical cross-linking
copolymerization reaction was investigated with the results shown in Fig.6. As is evident from Fig.6, performing the radical cross-linking copolymerization reaction at the initiators' decomposition temperature improves the process effectivity and the high degree of cross-linking. Temperatures at 80-900C and above are causing destructions and additional oxidation reactions which is naturally undesirable.
Fig. 6. Influence of temperature on cross-linking. mchitosan=0.35 g, VP=2.4 mol/1, 4VP=0.2 mol/1, t=150 min., AIBN=0.15 mol/l, Solvent=75 ml.
Thus, a new method was developed for the cross-linking degree and efficacy, as well as the optimal homopolymerization conditions for the chitosan-block-co-poly-4-
vinylpyridine-co-poly-N-vinylpyridine-copoly-N-vinylpyrrolidone cross-linked
copolymer. It revealed that at 60-700C within 150 min., the cross-linking degree (258%) and
the effectivity (17-19%) were max., while homopolymerization rate (18-20%) was min. in the cross-linking copolymerization reaction in the presence of 75 ml of 2% CH3COOH solvent, 0.35 g of chitosan and 2.4 mol/l of N-vinylpyrrolidone and 0.2 mol/l of 4-vinylpyridine.
CH3
1 3
CH3
1 3
H3C-C N=N C CH3 60;7°°V 2H3C-C
I I
C=N N=N
CH2
n-Ch CH
Q CH2/=\
°CH2P
CH
H2C
chqk
HC-N1 CH2
n^ch
CH2 HC-N
Q
Fig. 7. A schematic description of the cross-linking copolymerization reaction of the 4-vinylpyridine and the N-vinylpyrrolidone to chitosan.
The oxidizing agent apparently attacks the chitosan backbone, and free radicals arise on the glucoside ring directly followed by the monomer attacking this center which leads to
The quaternization and swelling behaviour of chitosan cross-linked poly-4-vinylpyridine-co-poly-N-vinylpyrrolidone
The quaternization of cross-linked copolymer with dimethylsulfate in the alkaline environment was compared with chitosan. It was established that the increased degree of macromolecule polarization, either in chitosan and cross-linked copolymer, results in the growth of quaternization. This results in a 4751% water diffusion. By adding max. calculated dimethyl sulfate to the content, the solubility of cross-linked copolymer rises as well. This tendency can be adjusted depending on the application area of the material. It found
the formation of the PVP-P4VP side chain [18]. Two possible mechanisms in the grafting reaction could be illustrated in the following Fig.7.
that the swelling of cross-linked copolymer increases spontaneously within 5-6 hours and the saturation occurs in 9-10 hours. Also, it was discovered that the swelling rate heavily depends on the molar ratio of monomers in the composition. The optimal hydrophilicity was provided with 62% and 38% of the 4-vinylpyridine and N-vinylpyrrolidone residues in the composition, respectively. Swelling degree was checked in acidic, neutral and alkaline buffer environments which varied at pH 2.5> pH 11> pH 7-8. The results obtained indicate that the transportation of the drugs to appropriate environments turns out to be possible.
Acknowledgements
The work has been supported by the Science Development Foundation under the President of the Republic of Azerbaijan- Grant № EiF-KETPL-2-2015-1(25)-56/22/4
REFERENCES
1. Gupta K.C., Ravikumar M.N.V. J. Mater. Sci. Rev. Macromol. Chem.Phys. 2000, vol. 40, p. 273-308.
2. Peter M.G. in: A. Steinbüchel, R.H. Marchessault (Eds.). Biopolymers for Medical and Pharmaceutical Applications, WileyVCH, Weinheim, 2005, pp. 419-512.
3. Shemshadi R., Zeynalov N.A., Tapdiqov Sh.Z. et al. Removal of Cadmium (II) by Natural Absorbents. Kimya Problemleri - Chemical Problems. 2009, no. 3, pp. 586- 589. (In Azerbaijan).
4. Kozo O., Yui Y., Okuyama K. Three D structures of chitosan. Int. J. Biol. Macromol. 2004, vol.34, isses 1-2, pp. 1-8.
5. Winterowd J.G., Sandford P.A., in: A.M. Stephen (Ed.), Food Polysaccharides and Their Applications, Marcel Dekker, New York, 1995, pp. 441-462.
6. Einbu A., Naess S.N., Elgsaeter A., Varum K.M. Solution Properties of Chitin in Alkali
Biomacromolecules. 2004, vol. 5, no. 5, 2048-2054.
7. Tapdiqov Sh.Z., Zeynalov N.A., Ahmedov I.D., Nurullaev Q.Q., Mamedova S.Q. Analysis Of Trypsin Immobilization On Metal Complexes With Poly-N-Vinylpyrrolidone. Kimya Problemleri -Chemical Problems. 2010, no. 3, pp. 406-411. (In Azerbaijan).
8. Vincendon M., in: C.J. Brine, P.A. Sandford, J.P. Zikakis (Eds.),Advances in Chitin and Chitosan, Elsevier, London and New York, 1992, pp. 556564.
9. Muzzarelli R.A.A., Guerrieri M., Goteri G., Muzzarelli C., Armen T., Ghiselli R., Cornelissen M. The biocompatibility of dibutyryl chitin in the context of wound dressings. Biomaterials. 2005, vol. 26, issue 29, pp. 5844-5854.
10. Kakizaki M., Shoji T., Tsutsumi A., Hideshima T., in: R.A.A.Muzzarelli, C. Jeuniaux, G.W. Gooday (Eds.), Chitin in Nature andTechnology, Plenum Press, New York, 1986, pp. 398-402.
11. Bagheri-Khoulenjani S, Taghizadeh S.M., Mirzadeh H. An investigation on the short-term biodegradability of chitosan with various molecular weights and degrees of deacetylation. Carbohydr. Polym., 2009, vol. 78, pp. 773-778.
12. Vandevord, P.J., Matthew H.W.T., Desilva S.P., Mayton L, Wu B., Wooley P.H. Evaluation of the biocompatibility of a chitosan scaffold in mice. J. Biomed. Mater. Res., 2002, vol. 59, pp. 585-590.
13. Chatelet C., Damour O., Domard A. Influence of the degree of acetylation on some biological properties of
chitosan films. Biomaterials, 2001, vol. 22, pp. 261-268.
14. Smith J. E. W., Dornish M. Effect of chitosan on epithelial cell tight junctions. Pharm. Res., 2004, vol.21, pp. 43-49.
15. Okamoto Y., Kawakami K., Miyatake K., Morimoto M., Shigemasa Y., Minami S. Analgesic effects of chitin and chitosan. Carbohydr. Polym., 2002, vol. 49, pp. 249-252.
16. Pourjavadi P., Mahdavinia G.R., Zohuriaan-Mehr M.J., Odian H. J ApplPolymSci. 2003, vol. 88, pp. 2048.
17. Yazdani-Pedram M., Lagos A., Campos N. Int J Polym Mater. 1992, vol. 18, pp. 25.
18. El-Tahlawy K., Huddson S.M., Graft copolymerization of hydroxyethyl methacrylate onto chitosan. Journal Appl. Polym. Sci., 2001, vol. 82, issue 3, pp. 683-702.
N-ViNiLPiRROLiDON Vd 4-ViMLPiRiDiMNXiTOZANA CALAQRADiKAL SOPOLiMERLd^MdSiNiN OPTiMAL ^dRAITiNiN TODQiQi
§.Z. Tapdiqov , N.A. Zeynalov , D.B. Tagiyev , S.F. Szforzliyeva*, E.M. Qasimov#,
A.F. Nurdüyev±, C.A. Sultanov
*Azdrbaycan Milli Elmldr Akademiyasi, akad. M.Nagiyev ad. Kataliz vd Qeyri-üzvi Kimya institutu AZ1143, Baki, H.Cavidpr.113, e-mail:[email protected] # Azdrbaycan Tibb Universiteti, Cdrrahliq vd Anesteziologiya §öbdsi AZ1022 Baki, S.Burgun küg.,167, e-mail: [email protected] ±AMEA Fizika institutu AZ 1143 Baki, H.Cavidküg., 117; e-mail: [email protected]
Ara^dirmada xitozani 4-vinilpiridin vd N-vinilpirrolidon i^tirakinda radikal sopolimerld^dirmdkld yeni tdbii-sintetik tdrkibli calaq sopolimerldr materiali alinmi^dir. Xitozana 4-vinilpiridin vd N-vinilpirrolidonun calaq edilmdsi ügün monomerldr i^tirakinda homogen fazada azobisizobutironitril inisiatoru ild radikal birgd calaq sopolimerld^md reaksiyalari aparilmi^dir. Calaq radikal sopolimerld^md prosesind dsas parametrldrin birgd tdsiri sistematik olaraq öyrdnilmi^dir. Xitozana monomerldrin calaq olunma ddrdcdsi (G%) vd calaq effektliyinin (E%) temperaturdan, xitozanin miqdarindan, inisiatorun qatiligindan, hdlledicinin hdcminddn, reaksiya müdddtinddn vd monomerldrin qatiligindan asili olaraq ddyi^mdsi tddqiq edilmi^dir. Müdyydn olunmu^dur ki, 60-700C-dd, 150 ddq. müdddtindd, 75 ml 2%-li CH3COOH hdlledici, 0.35 qr xitozan ild 2.4 mol/l N-vinilpirrolidon vd 0.2 mol/l 4-vinilpiridin i^tirakinda calaq sopolimerld^md reaksiyasinda G=258% vd E=17-19% max. olub, hdmginin homopolimerld^md ddrdcdsi 18-20% isd min. qiymdt ild xarakterizd olunur. H NMR, FTIR, SEM, X-Ray vd termoqravimetrik analiz metodlarinin tdtbiqi ild radikal calaq sopolimerld^mdsi reaksiyasinin dsasdn xitozandaki tsiklin qirilmasi ild ehtimal olunan mexanizmi tdklif olunmu^dur.
Agar sözlar: xitozan, calaq-sopolimerld^md, N-vinilpirrolidon, 4-vinilpiridin, radikal polimerld^md
ИССЛЕДОВАНИЕ ОПТИМАЛЬНЫХ УСЛОВИЙ ПРИВИТОЙ РАДИКАЛЬНОЙ СОПОЛИМЕРИЗАЦИИ N-ВИНИЛПИРРОЛИДОНА И 4-ВИНИЛПИРИДИНА НА ХИТОЗАН
Ш.З. Тапдыгов , Н.А. Зейналов, Д.Б. Тагиев , Э.М. Гасымов#, А.И. Маммедова ,
А.Ф. Нуралиев±, Ч.А. Султанов*
"Институт Катализа и Неорганической химии имени академика М. Нагиева Национальной АН Азербайджана, AZ1143 Баку, пр. Г.Джавида, 113, e-mail:[email protected] #Азербайджанский Медицинский Университет, Отделение Хирургии и Анестезиологии AZ1022 Бaку, ул. С.Вургуна 167, e-mail: [email protected] ± Институт Физики Национальной АН Азербайджана AZ1143 Баку, пр. Г.Джавида, 117; e-mail: azhep@ physics.ab.az
Радикальной сополимеризацией хитозана с участием 4-винилпиридина и N-винилпирролидона получены привитые сополимеры, содержащие новые натурально-синтетические материалы. Для прививки 4-винилпиридина и N-винилпирролидона на хитозан проведена реакция совместной радикальной и привитой сополимеризации в присутствии мономера в гомогенной фазе, инициированной азобисизобутиронитрилом. Было изучено совместное действие основных параметров на процесс привитой радикальной сополимеризации. Исследована зависимость степени прививки (G%) мономеров на хитозан и эффективность прививки (E%) от температуры, количества хитозана, концентрации инициатора, объема растворителя, времени реакции и концентрации мономеров. Установлено, что при температуре 60-700С, продолжительности 150 мин., в присутствии растворителя - 75 мл 2%-ной CH3COOH, реакция сополимеризации 0.35 г хитозана с 2.4 моль/л N-винилпирролидоном и 0.2 моль/л 4-винилпиридином характеризуется максимальными значениями степени прививки G = 258% и эффективности прививки E = 17-19 % и минимальным значением степени гомополимеризации 18-20%. Используя методы H NMR, FTIR, SEM, X-Ray и термографический анализ, предложен предполагаемый механизм радикальной привитой реакции сополимеризации, характеризующийся, в основном обрывом цикла хитозана.
Ключевые слова: хитозан, привитая сополимеризация, N-винилпирролидон, 4-винилпиридин, радикальная полимеризация